ABS/ASA Blend Print Settings: A Filazoo Setup Guide
Published by Filazoo Team
·5 min read
Printing Filazoo ABS/ASA blend for the first time? Start with 255 °C at the nozzle, 100 °C on the bed, 50 mm/s, a 0.20 mm layer height and the part-cooling fan off. Use an enclosure approved for your printer and a build surface suitable for ABS/ASA. Then tune a small part before committing to a full housing or prop.
This guide uses the starting profile and adjustment ranges supplied for Filazoo ABS/ASA Blend, 1.75 mm, 1 kg. These are setup recommendations, not a universal profile or a measured strength test. Other brands and formulations may need different settings.
ABS/ASA blend print settings at a glance
| Setting | Start here | Product guidance |
|---|---|---|
| Nozzle temperature | 255 °C | 240–270 °C |
| Bed temperature | 100 °C | 90–110 °C |
| Print speed | 50 mm/s | 40–80 mm/s |
| First-layer speed | 20–30 mm/s | Check adhesion before increasing speed |
| Layer height | 0.20 mm | Starting point with a 0.4 mm nozzle |
| Part-cooling fan | 0% | 0–20%; use only as needed for the geometry |
| Nozzle size | 0.4 mm | 0.4 mm or larger |
| Enclosure | Strongly recommended | Use a printer-approved enclosure and ventilation setup |
Stay within your printer, hotend and build-plate limits. Fan percentages here refer to the part-cooling fan; keep the hotend heatsink fan operating as the printer manufacturer specifies.
Check your printer before choosing the filament
A heated bed is required. An enclosure helps keep conditions around the part steady, particularly for broad bases and tall walls. A high maximum nozzle temperature alone does not establish compatibility: the printer must also support the bed temperature, material and operating environment.
For example, Bambu Lab's A1 quick-start guide lists ABS and ASA as not recommended. Do not assume a generic ABS profile makes an open printer suitable, or add an enclosure contrary to the printer manufacturer's instructions. On a compatible enclosed machine, begin with its supported ABS/ASA material preset and enter the Filazoo starting values above. Save your changes as a separate profile.
Plan ventilation alongside temperature control. An enclosure by itself is not proof of adequate emissions control; follow the printer manufacturer's guidance and use appropriate extraction or ventilation for the workspace.
Run a small first print
- Choose a useful test. Print a small section of your actual model with a corner, a vertical wall and any critical hole or mating feature. A decorative cube alone will not check the fit of your enclosure lid.
- Prepare the plate. Clean it using the plate manufacturer's method, check the first-layer calibration, and use an adhesive or release layer where that surface requires one.
- Record the starting conditions. Note the printer, plate, nozzle, filament color and the settings in the table. Keep the setup consistent between trials.
- Inspect the first layer. If lines do not attach evenly, resolve first-layer calibration and surface preparation before changing the whole profile.
- Let the part cool before assessing it. Check for lifted corners, visible splits, rough surfaces and fit. Photograph the result and change one relevant setting for the next trial.
Troubleshoot the symptom you actually see
Corners lift later in the print
Later lifting points you toward thermal contraction as well as bed adhesion. Check drafts, enclosure use and unnecessary part cooling; consider a brim for a broad base. Avoid treating every lifted corner as a reason to raise nozzle temperature. The warping troubleshooting guide explains how to distinguish first-layer problems from lifting that develops later.
Walls split between layers
Review cooling, nozzle temperature and extrusion consistency. Use a modest trial within the product's stated range, then inspect a new sample. More infill will not repair poor bonding between layers. See the layer adhesion guide for a fuller diagnosis.
Bridges or small overhangs sag
After establishing good adhesion, trial a small amount of part cooling within the 0–20% range for those features. Recheck the surrounding walls for splitting. You may also improve orientation or supports instead of increasing cooling across the entire print.
Extrusion pops or the surface becomes inconsistent
Moisture is one possible cause, alongside temperature and extrusion problems. Filazoo's current product guidance lists 70–80 °C for 4–6 hours when drying is required. Confirm that the spool and dryer are rated for the chosen temperature; follow any instructions supplied with your batch if they differ. Store the filament sealed with desiccant afterward. A passive storage box helps keep dry filament dry but is not a substitute for drying wet material. Read the filament drying guide before choosing equipment.
Validate the finished part
For a housing, check the lid, screw locations and cable openings. For a workshop fixture, check repeatability over several uses. For a painted prop, test primer and paint on a small sample before finishing the full model. Keep the successful profile with those notes so the next print starts from evidence.
Nozzle temperature is a printing setting, not the part's service-temperature rating. This guide does not establish a heat rating, outdoor lifetime or load capacity for the blend. For material selection, see ABS vs ASA vs ABS/ASA blend.
Ready to choose a color?
View Filazoo ABS/ASA Blend filament and current color availability. Use the selected variant's delivery estimate when planning your project.
Sources and scope
The numeric settings above come from Filazoo's product guidance. General troubleshooting references: Prusa: warping, Prusa: layer separation, Prusa: drying filament, Bambu Lab: A1 quick-start guide, and NIOSH: approaches to safe 3D printing. Other manufacturers' material properties are not specifications for the Filazoo blend.
Keep exploring
Related articles
ABS/ASA
ABS vs ASA vs ABS/ASA Blend: Which Filament Fits Your Part?
Compare ABS, ASA and ABS/ASA blend for housings, fixtures, outdoor projects and painted props, with practical checks before...
Multimaterial
PLA and PETG Support Interfaces: Cleaner Removal, Important Limits
Learn when PLA and PETG can separate as support interfaces, why shared-nozzle purging matters and how to test...
Decorative Prints
Translucent PETG: How to Plan Light-Diffusing Decorative Prints
Plan translucent PETG panels and decorative covers. Compare wall thickness, print direction and lighting while avoiding unrealistic glass-clear...
Filazoo community
Ask a question, share a printing tip, or tell us what worked for your project.